Specification process of anti-static PVC floor construction

Aug 18, 2020 Leave a message

Specification process of anti-static PVC floor construction:

   1. Delineation of the reference line should be reasonably determined according to the geometric shape of the room.

  2, the conductive copper foil grid should be laid according to the ground grid layout. The vertical and horizontal intersection of the copper foil should be at the center of the veneer. The laying of copper foil strips should be straight, not curled, or interrupted. The copper foil strip connected to the grounding terminal should be left with sufficient length.

  3. Configure conductive glue: The carbon black and glue should be configured in a weight ratio of 1:100 and mixed evenly.

  4. Brush glue: It should be on the ground and on the conductive copper foil that has been laid. The coating should be uniform and comprehensive, and it should be dried naturally after coating.

5. Paving the veneer: When the dehydrated ground is dried until it is not sticky, the paving should be started. When paving, the two right-angle edges of the veneer should be aligned with the reference line, and the paving should be fast and fast. There should be a gap of 1-2mm between the board and the board, and the width of the gap should be kept basically the same. Use a rubber hammer to evenly hit the board surface, and check the edge of the side to ensure that the adhesion is firm. The edge of the ground should be pave and patched with non-standard veneer ,The non-standard veneer is cut by the standard veneer with a cutter.

  6. When paving the ground terminal, the copper foil strip connected to the ground terminal should be led out, and the ground terminal should be firmly connected by soldering or crimping. Then continue to pave the panel.

  7. After the whole room has been pasted, a slotting machine should be used to open the welding groove along the seam of the veneer. The groove line should be straight and even, and the groove width should be 3±0.2mm.

   8. The plastic welding gun is used for thermoplastic welding at the welding groove, so that the board and the board are integrated. Welding excess should be cut flat with a sharp knife, but the surface of the veneer must not be scratched.

   9. The construction of the grounding system should include the application of conductive adhesive layer, conductive copper foil ground net, grounding copper foil, grounding terminal, grounding down conductor, grounding body, etc. Except for the provisions of this chapter, the rest shall comply with the provisions of this code.

  10. After the paving operation is completed, the floor should be cleaned and coated with anti-static wax for protection.